WO2002093240A1 - Liquid crystal display device and optical laminate - Google Patents
Liquid crystal display device and optical laminate Download PDFInfo
- Publication number
- WO2002093240A1 WO2002093240A1 PCT/JP2002/004663 JP0204663W WO02093240A1 WO 2002093240 A1 WO2002093240 A1 WO 2002093240A1 JP 0204663 W JP0204663 W JP 0204663W WO 02093240 A1 WO02093240 A1 WO 02093240A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- liquid crystal
- display device
- crystal display
- layer
- plastic substrate
- Prior art date
Abstract
Description
Claims