WO2007084317A2 - Silicon-rich silicon nitrides as etch stops in mems manufacture - Google Patents
Silicon-rich silicon nitrides as etch stops in mems manufacture Download PDFInfo
- Publication number
- WO2007084317A2 WO2007084317A2 PCT/US2007/000698 US2007000698W WO2007084317A2 WO 2007084317 A2 WO2007084317 A2 WO 2007084317A2 US 2007000698 W US2007000698 W US 2007000698W WO 2007084317 A2 WO2007084317 A2 WO 2007084317A2
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- layer
- silicon nitride
- sacrificial layer
- unreleased
- mems device
- Prior art date
Abstract
The fabrication of a MEMS device such as an interferometric modulator is improved by employing an etch stop layer 104b between a sacrificial layer and an electrode 14a, 14b, 14c. The etch stop 104b may reduce undesirable over-etching of the sacrificial layer and the electrode 14a, 14b, 14c. The etch stop layer 104b may also serve as a barrier layer, buffer layer, and/or template layer. The etch stop layer 104b may include silicon-rich silicon nitride.
Description
SILICON-RICH SILICON NITRIDES AS ETCH STOPS IN MEMS
MANUFACTURE
FIELD OF THE INVENTION
[0001 J Microelectromechanical systems (MEMS) include micro mechanical elements, actuators, and electronics. Micromechanical elements may be created using deposition, etching, and or other micromachining processes that etch away parts of substrates and/or deposited material layers or that add layers to form electrical and electromechanical devices. One type of MEMS device is called an interferometric modulator. As used herein, the term interferometric modulator or interferometric light modulator refers to a device that selectively absorbs and/or reflects light using the principles of optical interference. In certain embodiments, an interferometric modulator may comprise a pair of conductive plates, one or both of which may be transparent and/or reflective in whole or part and capable of relative motion upon application of an appropriate electrical signal. In a particular embodiment, one plate may comprise a stationary layer deposited on a substrate and the other plate may comprise a metallic membrane separated from the stationary layer by an air gap. As described herein in more detail, the position of one plate in relation to another can change the optical interference of light incident on the interferometric modulator. Such devices have a wide range of applications, and it would be beneficial in the art to utilize and/or modify the characteristics of these types of devices so that their features can be exploited in improving existing products and creating new products that have not yet been developed.
SUMMARY
[0002] One embodiment disclosed herein includes an unreleased MEMS device, comprising a silicon nitride layer positioned between a sacrificial layer and an electrode layer, wherein the electrode layer is adapted to be movable upon removal of the sacrificial layer and the ratio of silicon to nitrogen in the silicon nitride layer is greater than 3:4.
[0003] Another embodiment disclosed herein includes an unreleased interferometric modulator, comprising an etch stop layer positioned between a sacrificial layer and a metal mirror layer, wherein the metal mirror layer is adapted to be movable
upon removal of the sacrificial layer and the etch stop layer is adapted to be substantially completely removed upon exposure to XeF2 for less than about 10 minutes.
[0004] Another embodiment disclosed herein includes an unreleased MEMS device, comprising a silicon nitride layer positioned between a sacrificial layer and an electrode layer, wherein the electrode layer is adapted to be movable upon removal of the sacrificial layer, the silicon nitride layer is adapted to be substantially completely removed upon exposure to a first etchant that is adapted to substantially completely remove the sacrificial layer, and the silicon nitride layer is adapted to be substantially resistant to a second etchant that is adapted to substantially completely remove the electrode layer.
[0005] Another embodiment disclosed herein includes an unreleased interferometric modulator, comprising means for reflecting light, means for supporting the reflecting means during interferometric modulator manufacture, and means for protecting the supporting means during etching of the reflecting means.
[0006] Another embodiment disclosed herein includes a method of manufacturing a MEMS device, comprising forming a sacrificial layer, forming an electrode layer, wherein the electrode layer is adapted to be movable upon removal of the sacrificial layer, forming a silicon nitride layer between the sacrificial layer and the electrode layer, wherein the ratio of silicon to nitrogen in the silicon nitride layer is greater than about 3:4, patterning the electrode layer, and removing the sacrificial layer.
[0007] Another embodiment disclosed herein includes a method of manufacturing a MEMS device, comprising forming a sacrificial layer, forming an electrode layer, wherein the electrode layer is adapted to be movable upon removal of the sacrificial layer, forming an etch stop layer between the sacrificial layer and the electrode layer, patterning the electrode layer, and removing the sacrificial layer and etch stop layer with a same etchant.
BRIEF DESCRIPTION OF THE DRAWINGS [0008] FIG. 1 is an isometric view depicting a portion of one embodiment of an interferometric modulator display in which a movable reflective layer of a first interferometric modulator is in a relaxed position and a movable reflective layer of a second interferometric modulator is in an actuated position.
[0009] FIG. 2 is a system block diagram illustrating one embodiment of an electronic device incorporating a 3x3 interferometric modulator display.
[0010] FIG. 3 is a diagram of movable mirror position versus applied voltage for one exemplary embodiment of an interferometric modulator of FIG. 1.
(00111 FIG. 4 is an illustration of a set of row and column voltages that may be used to drive an interferometric modulator display.
[0012] FIGS. 5A and 5B illustrate one exemplary timing diagram for row and column signals that may be used to write a frame of display data to the 3x3 interferometric modulator display of FIG. 2.
[0013] FIGS. 6A and 6B are system block diagrams illustrating an embodiment of a visual display device comprising a plurality of interferometric modulators.
[0014] FIG. 7 A is a cross section of the device of FIG. 1.
[0015] FIG. 7B is a cross section of an alternative embodiment of an interferometric modulator.
[0016] FIG. 7C is a cross section of another alternative embodiment of an interferometric modulator.
[0017] FIG 7D is a cross section of yet another alternative embodiment of an interferometric modulator.
[0018] FIG. 7E is a cross section of an additional alternative embodiment of an interferometric modulator.
[0019] FIG. 8 is a cross section of an embodiment of an unreleased interferometric modulator.
[0020] FIGS. 9A-9E are cross-sections illustrating the initial process steps in an embodiment of a method for making an array of interferometric modulators.
[0021] FIGS. 10A- 1OH are cross-sections illustrating the later process steps in the embodiment of a method for making an array of interferometric modulators.
[0022] FIG. 11 is a graph depicting XeF2 etch step height as a function of silicon-rich silicon nitride refractive index.
DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS [0023] The following detailed description is directed to certain specific embodiments of the invention. However, the invention can be embodied in a multitude of different ways. In this description, reference is made to the drawings wherein like parts are designated with like numerals throughout. As will be apparent from the following description, the embodiments may be implemented in any device that is configured to
display an image, whether in motion (e.g., video) or stationary (e.g., still image), and whether textual or pictorial. More particularly, it is contemplated that the embodiments may be implemented in or associated with a variety of electronic devices such as, but not limited to, mobile telephones, wireless devices, personal data assistants (PDAs), hand-held or portable computers, GPS receivers/navigators, cameras, MP3 players, camcorders, game consoles, wrist watches, clocks, calculators, television monitors, flat panel displays, computer monitors, auto displays (e.g., odometer display, etc.), cockpit controls and/or displays, display of camera views (e.g., display of a rear view camera in a vehicle), electronic photographs, electronic billboards or signs, projectors, architectural structures, packaging, and aesthetic structures (e.g., display of images on a piece of jewelry). MEMS devices of similar structure to those described herein can also be used in non-display applications such as in electronic switching devices.
[0024] An embodiment provides a method for making an interferometric modulator that involves the use of an etch stop between an upper electrode or reflective layer and a sacrificial layer. The etch stop can be used to reduce undesirable over-etching of the sacrificial layer and the upper electrode or mirror layer. The etch stop layer may also serve as a barrier layer, buffer layer, and/or template layer. The etch stop layer is advantageously silicon-rich silicon nitride, which can be cleanly removed simultaneously with removal of the sacrificial layer.
[0025] One interferometric modulator display embodiment comprising an interferometric MEMS display element is illustrated in Figure 1. In these devices, the pixels are in either a bright or dark state. In the bright ("on" or "open") state, the display element reflects a large portion of incident visible light to a user. When in the dark ("off or "closed") state, the display element reflects little incident visible light to the user. Depending on the embodiment, the light reflectance properties of the "on" and "off states may be reversed. MEMS pixels can be configured to reflect predominantly at selected colors, allowing for a color display in addition to black and white.
[0026] Figure 1 is an isometric view depicting two adjacent pixels in a series of pixels of a visual display, wherein each pixel comprises a MEMS interferometric modulator. In some embodiments, an interferometric modulator display comprises a row/column array of these interferometric modulators. Each interferometric modulator includes a pair of reflective layers positioned at a variable and controllable distance from each other to form a resonant optical cavity with at least one variable dimension. In one
embodiment, one of the reflective layers may be moved between two positions. In the first position, referred to herein as the relaxed position, the movable reflective layer is positioned at a relatively large distance from a fixed partially reflective layer. In the second position, referred to herein as the actuated position, the movable reflective layer is positioned more closely adjacent to the partially reflective layer. Incident light that reflects from the two layers interferes constructively or destructively depending on the position of the movable reflective layer, producing either an overall reflective or non-reflective state for each pixel.
[0027] The depicted portion of the pixel array in Figure 1 includes two adjacent interferometric modulators 12a and 12b. In the interferometric modulator 12a on the left, a movable reflective layer 14a is illustrated in a relaxed position at a predetermined distance from an optical stack 16a, which includes a partially reflective layer. In the interferometric modulator 12b on the right, the movable reflective layer 14b is illustrated in an actuated position adjacent to the optical stack 16b.
[0028] The optical stacks 16a and 16b (collectively referred to as optical stack 16), as referenced herein, typically comprise of several fused layers, which can include an electrode layer, such as indium tin oxide (ITO), a partially reflective layer, such as chromium, and a transparent dielectric. The optical stack 16 is thus electrically conductive, partially transparent and partially reflective, and may be fabricated, for example, by depositing one or more of the above layers onto a transparent substrate 20. The partially reflective layer can be formed from a variety of materials that are partially reflective such as various metals, semiconductors, and dielectrics. The partially reflective layer can be formed of one or more layers of materials, and each of the layers can be formed of a single material or a combination of materials.
[0029] In some embodiments, the layers of the optical stack are patterned into parallel strips, and may form row electrodes in a display device as described further below. The movable reflective layers 14a, 14b may be formed as a series of parallel strips of a deposited metal layer or layers (orthogonal to the row electrodes of 16a, 16b) deposited on top of posts 18 and an intervening sacrificial material deposited between the posts 18. When the sacrificial material is etched away, the movable reflective layers 14a, 14b are separated from the optical stacks 16a, 16b by a defined gap 19. A highly conductive and reflective material such as aluminum may be used for the reflective layers 14, and these strips may form column electrodes in a display device.
[0030] With no applied voltage, the cavity 19 remains between the movable reflective layer 14a and optical stack 16a, with the movable reflective layer 14a in a mechanically relaxed state, as illustrated by the pixel 12a in Figure 1. However, when a potential difference is applied to a selected row and column, the capacitor formed at the intersection of the row and column electrodes at the corresponding pixel becomes charged, and electrostatic forces pull the electrodes together. If the voltage is high enough, the movable reflective layer 14 is deformed and is forced against the optical stack 16. A dielectric layer (not illustrated in this Figure) within the optical stack 16 may prevent shorting and control the separation distance between layers 14 and 16, as illustrated by pixel 12b on the right in Figure 1. The behavior is the same regardless of the polarity of the applied potential difference. In this way, row/column actuation that can control the reflective vs. non-reflective pixel states is analogous in many ways to that used in conventional LCD and other display technologies.
[0031] Figures 2 through 5B illustrate one exemplary process and system for using an array of interferometric modulators in a display application.
[0032] Figure 2 is a system block diagram illustrating one embodiment of an electronic device that may incorporate aspects of the invention. In the exemplary embodiment, the electronic device includes a processor 21 which may be any general purpose single- or multi-chip microprocessor such as an ARM, Pentium®, Pentium II®, Pentium III®, Pentium IV®, Pentium® Pro, an 8051, a MIPS®, a Power PC®, an ALPHA®, or any special purpose microprocessor such as a digital signal processor, microcontroller, or a programmable gate array. As is conventional in the art, the processor 21 may be configured to execute one or more software modules. In addition to executing an operating system, the processor may be configured to execute one or more software applications, including a web browser, a telephone application, an email program, or any other software application.
[0033] In one embodiment, the processor 21 is also configured to communicate with an array driver 22. In one embodiment, the array driver 22 includes a row driver circuit 24 and a column driver circuit 26 that provide signals to a display array or panel 30. The cross section of the array illustrated in Figure 1 is shown by the lines 1-1 in Figure 2. For MEMS interferometric modulators, the row/column actuation protocol may take advantage of a hysteresis property of these devices illustrated in Figure 3. It may require, for example, a 10 volt potential difference to cause a movable layer to deform from the
relaxed state to the actuated state. However, when the voltage is reduced from that value, the movable layer maintains its state as the voltage drops back below 10 volts. In the exemplary embodiment of Figure 3, the movable layer does not relax completely until the voltage drops below 2 volts. There is thus a range of voltage, about 3 to 7 V in the example illustrated in Figure 3, where there exists a window of applied voltage within which the device is stable in either the relaxed or actuated state. This is referred to herein as the "hysteresis window" or "stability window." For a display array having the hysteresis characteristics of Figure 3, the row/column actuation protocol can be designed such that during row strobing, pixels in the strobed row that are to be actuated are exposed to a voltage difference of about 10 volts, and pixels that are to be relaxed are exposed to a voltage difference of close to zero volts. After the strobe, the pixels are exposed to a steady state voltage difference of about 5 volts such that they remain in whatever state the row strobe put them in. After being written, each pixel sees a potential difference within the "stability window" of 3-7 volts in this example. This feature makes the pixel design illustrated in Figure 1 stable under the same applied voltage conditions in either an actuated or relaxed pre-existing state. Since each pixel of the interferometric modulator, whether in the actuated or relaxed state, is essentially a capacitor formed by the fixed and moving reflective layers, this stable state can be held at a voltage within the hysteresis window with almost no power dissipation. Essentially no current flows into the pixel if the applied potential is fixed.
[0034] In typical applications, a display frame may be created by asserting the set of column electrodes in accordance with the desired set of actuated pixels in the first row. A row pulse is then applied to the row 1 electrode, actuating the pixels corresponding to the asserted column lines. The asserted set of column electrodes is then changed to correspond to the desired set of actuated pixels in the second row. A pulse is then applied to the row 2 electrode, actuating the appropriate pixels in row 2 in accordance with the asserted column electrodes. The row 1 pixels are unaffected by the row 2 pulse, and remain in the state they were set to during the row 1 pulse. This may be repeated for the entire series of rows in a sequential fashion to produce the frame. Generally, the frames are refreshed and/or updated with new display data by continually repeating this process at some desired number of frames per second. A wide variety of protocols for driving row and column electrodes of pixel arrays to produce display frames are also well known and may be used in conjunction with the present invention.
[0035] Figures 4, 5A, and 5B illustrate one possible actuation protocol for creating a display frame on the 3x3 array of Figure 2. Figure 4 illustrates a possible set of column and row voltage levels that may be used for pixels exhibiting the hysteresis curves of Figure 3. hi the Figure 4 embodiment, actuating a pixel involves setting the appropriate column to -Vt>ias> and the appropriate row to +ΔV, which may correspond to -5 volts and +5 volts respectively Relaxing the pixel is accomplished by setting the appropriate column to +Vbias5 and the appropriate row to the same +ΔV, producing a zero volt potential difference across the pixel. In those rows where the row voltage is held at zero volts, the pixels are stable in whatever state they were originally in, regardless of whether the column is at +Vbias> or -Vbjas. As is also illustrated in Figure 4, it will be appreciated that voltages of opposite polarity than those described above can be used, e.g., actuating a pixel can involve setting the appropriate column to +VbiaS:> and the appropriate row to — ΔV. In this embodiment, releasing the pixel is accomplished by setting the appropriate column to -Vbiasj and the appropriate row to the same -ΔV, producing a zero volt potential difference across the pixel.
[0036] Figure 5B is a timing diagram showing a series of row and column signals applied to the 3x3 array of Figure 2 which will result in the display arrangement illustrated in Figure 5A, where actuated pixels are non-reflective. Prior to writing the frame illustrated in Figure 5A, the pixels can be in any state, and in this example, all the rows are at 0 volts, and all the columns are at +5 volts. With these applied voltages, all pixels are stable in their existing actuated or relaxed states.
[0037] In the Figure 5A frame, pixels (1,1), (1,2), (2,2), (3,2) and (3,3) are actuated. To accomplish this, during a "line time" for row 1, columns 1 and 2 are set to -5 volts, and column 3 is set to +5 volts. This does not change the state of any pixels, because all the pixels remain in the 3-7 volt stability window. Row 1 is then strobed with a pulse that goes from 0, up to 5 volts, and back to zero. This actuates the (1,1) and (1,2) pixels and relaxes the (1,3) pixel. No other pixels in the array are affected. To set row 2 as desired, column 2 is set to -5 volts, and columns 1 and 3 are set to +5 volts. The same strobe applied to row 2 will then actuate pixel (2,2) and relax pixels (2,1) and (2,3). Again, no other pixels of the array are affected. Row 3 is similarly set by setting columns 2 and 3 to -5 volts, and column 1 to +5 volts. The row 3 strobe sets the row 3 pixels as shown in Figure 5A. After writing the frame, the row potentials are zero, and the column potentials can remain at either +5 or -5 volts, and the display is then stable in the arrangement of
Figure 5A. It will be appreciated that the same procedure can be employed for arrays of dozens or hundreds of rows and columns. It will also be appreciated that the timing, sequence, and levels of voltages used to perform row and column actuation can be varied widely within the general principles outlined above, and the above example is exemplary only, and any actuation voltage method can be used with the systems and methods described herein.
[0038] Figures 6A and 6B are system block diagrams illustrating an embodiment of a display device 40. The display device 40 can be, for example, a cellular or mobile telephone. However, the same components of display device 40 or slight variations thereof are also illustrative of various types of display devices such as televisions and portable media players.
[0039J The display device 40 includes a housing 41, a display 30, an antenna 43, a speaker 44, an input device 48, and a microphone 46. The housing 41 is generally formed from any of a variety of manufacturing processes as are well known to those of skill in the art, including injection molding, and vacuum forming. In addition, the housing 41 may be made from any of a variety of materials, including but not limited to plastic, metal, glass, rubber, and ceramic, or a combination thereof. In one embodiment the housing 41 includes removable portions (not shown) that may be interchanged with other removable portions of different color, or containing different logos, pictures, or symbols.
[0040] The display 30 of the exemplary display device 40 may be any of a variety of displays, including a bi-stable display, as described herein. In other embodiments, the display 30 includes a flat-panel display, such as plasma, EL, OLED, STN LCD, or TFT LCD as described above, or a non-flat-panel display, such as a CRT or other tube device, as is well known to those of skill in the art. However, for purposes of describing the present embodiment, the display 30 includes an interferon! etric modulator display, as described herein.
[0041] The components of one embodiment of exemplary display device 40 are schematically illustrated in Figure 6B. The illustrated exemplary display device 40 includes a housing 41 and can include additional components at least partially enclosed therein. For example, in one embodiment, the exemplary display device 40 includes a network interface 27 that includes an antenna 43 which is coupled to a transceiver 47. The transceiver 47 is connected to a processor 21, which is connected to conditioning hardware 52. The conditioning hardware 52 may be configured to condition a signal (e.g., filter a
signal). The conditioning hardware 52 is connected to a speaker 45 and a microphone 46. The processor 21 is also connected to an input device 48 and a driver controller 29. The driver controller 29 is coupled to a frame buffer 28, and to an array driver 22, which in turn is coupled to a display array 30. A power supply 50 provides power to all components as required by the particular exemplary display device 40 design.
[0042] The network interface 27 includes the antenna 43 and the transceiver 47 so that the exemplary display device 40 can communicate with one ore more devices over a network. In one embodiment the network interface 27 may also have some processing capabilities to relieve requirements of the processor 21. The antenna 43 is any antenna known to those of skill in the art for transmitting and receiving signals. In one embodiment, the antenna transmits and receives RF signals according to the IEEE 802.1 1 standard, including IEEE 802.1 l(a), (b), or (g). In another embodiment, the antenna transmits and receives RF signals according to the BLUETOOTH standard. In the case of a cellular telephone, the antenna is designed to receive CDMA, GSM, AMPS or other known signals that are used to communicate within a wireless cell phone network. The transceiver 47 pre- processes the signals received from the antenna 43 so that they may be received by and further manipulated by the processor 21. The transceiver 47 also processes signals received from the processor 21 so that they may be transmitted from the exemplary display device 40 via the antenna 43.
[0043] In an alternative embodiment, the transceiver 47 can be replaced by a receiver. In yet another alternative embodiment, the network interface 27 can be replaced by an image source, which can store or generate image data to be sent to the processor 21. For example, the image source can be a digital video disc (DVD) or a hard-disc drive that contains image data, or a software module that generates image data.
[0044] The processor 21 generally controls the overall operation of the exemplary display device 40. The processor 21 receives data, such as compressed image data from the network interface 27 or an image source, and processes the data into raw image data or into a format that is readily processed into raw image data. The processor 21 then sends the processed data to the driver controller 29 or to the frame buffer 28 for storage. Raw data typically refers to the information that identifies the image characteristics at each location within an image. For example, such image characteristics can include color, saturation, and gray-scale level.
[0045] In one embodiment, the processor 21 includes a microcontroller, CPU, or logic unit to control operation of the exemplary display device 40. The conditioning hardware 52 generally includes amplifiers and filters for transmitting signals to the speaker 45, and for receiving signals from the microphone 46. The conditioning hardware 52 may be discrete components within the exemplary display device 40, or may be incorporated within the processor 21 or other components.
[0046] The driver controller 29 takes the raw image data generated by the processor 21 either directly from the processor 21 or from the frame buffer 28 and reformats the raw image data appropriately for high speed transmission to the array driver 22. Specifically, the driver controller 29 reformats the raw image data into a data flow having a raster-like format, such that it has a time order suitable for scanning across the display array 30. Then the driver controller 29 sends the formatted information to the array driver 22. Although a driver controller 29, such as a LCD controller, is often associated with the system processor 21 as a stand-alone Integrated Circuit (IC), such controllers may be implemented in many ways. They may be embedded in the processor 21 as hardware, embedded in the processor 21 as software, or fully integrated in hardware with the array driver 22.
[0047] Typically, the array driver 22 receives the formatted information from the driver controller 29 and reformats the video data into a parallel set of waveforms that are applied many times per second to the hundreds and sometimes thousands of leads coming from the display's x-y matrix of pixels.
[0048] In one embodiment, the driver controller 29, array driver 22, and display array 30 are appropriate for any of the types of displays described herein. For example, in one embodiment, the driver controller 29 is a conventional display controller or a bi-stable display controller (e.g., an interferometric modulator controller). In another embodiment, the array driver 22 is a conventional driver or a bi-stable display driver (e.g., an interferometric modulator display). In one embodiment, the driver controller 29 is integrated with the array driver 22. Such an embodiment is common in highly integrated systems such as cellular phones, watches, and other small area displays. In yet another embodiment, display array 30 is a typical display array or a bi-stable display array (e.g., a display including an array of interferometric modulators).
[0049] The input device 48 allows a user to control the operation of the exemplary display device 40. In one embodiment, the input device 48 includes a keypad,
such as a QWERTY keyboard or a telephone keypad^ a button, a switch, a touch-sensitive screen, a pressure- or heat-sensitive membrane. In one embodiment, the microphone 46 is an input device for the exemplary display device 40. When the microphone 46 is used to input data to the device, voice commands may be provided by a user for controlling operations of the exemplary display device 40.
[0050] The power supply 50 can include a variety of energy storage devices as are well known in the art. For example, in one embodiment, the power supply 50 is a rechargeable battery, such as a nickel-cadmium battery or a lithium ion battery. In another embodiment, the power supply 50. is a renewable energy source, a capacitor, or a solar cell, including a plastic solar cell, and solar-cell paint. In another embodiment, the power supply 50 is configured to receive power from a wall outlet.
[0051] In some implementations control programmability resides, as described above, in a driver controller which can be located in several places in the electronic display system. In some cases control programmability resides in the array driver 22. Those of skill in the art will recognize that the above-described optimization may be implemented in any number of hardware and/or software components and in various configurations.
[0052] The details of the structure of interferometric modulators that operate in accordance with the principles set forth above may vary widely. For example, Figures 7A- 7E illustrate five different embodiments of the movable reflective layer 14 and its supporting structures. Figure 7 A is a cross section of the embodiment of Figure 1, where a strip of metal material 14 is deposited on orthogonally extending supports 18. In Figure 7B, the moveable reflective layer 14 is attached to supports 18 at the corners only, on tethers 32. In Figure 7C, the moveable reflective layer 14 is suspended from a deformable layer 34, which may comprise a flexible metal. The deformable layer 34 connects, directly or indirectly, to the substrate 20 around the perimeter of the deformable layer 34. The connections are herein referred to as supports or posts 18. The embodiment illustrated in Figure 7D has supports 18 including support post plugs 42 upon which the deformable layer 34 rests. The movable reflective layer 14 remains suspended over the cavity, as in Figures 7A-7C, but the deformable layer 34 does not form the support posts by filling holes between the deformable layer 34 and the optical stack 16. Rather, the support posts are formed of a planarization material, which is used to form support post plugs 42. The embodiment illustrated in Figure 7E is based on the embodiment shown in Figure 7D, but may also be adapted to work with any of the embodiments illustrated in Figures 7A-7C as
well as additional embodiments not shown. In the embodiment shown in Figure 7E, an extra layer of metal or other conductive material has been used to form a bus structure 44. This allows signal routing along the back of the interferometric modulators, eliminating a number of electrodes that may otherwise have had to be formed on the substrate 20.
[0053] In embodiments such as those shown in Figures 7A-7E, the interferometric modulators function as direct-view devices, in which images are viewed from the front side of the transparent substrate 20, the side opposite to that upon which the modulator is arranged. In these embodiments, the reflective layer 14 optically shields the portions of the interferometric modulator on the side of the reflective layer opposite the substrate 20, including the deformable layer 34. This allows the shielded areas to be configured and operated upon without negatively affecting the image quality. Such shielding allows the bus structure 44 in Figure 7E, which provides the ability to separate the optical properties of the modulator from the electromechanical properties of the modulator, such as addressing and the movements that result from that addressing. This separable modulator architecture allows the structural design and materials used for the electromechanical aspects and the optical aspects of the modulator to be selected and to function independently of each other. Moreover, the embodiments shown in Figures 7C-7E have additional benefits deriving from the decoupling of the optical properties of the reflective layer 14 from the mechanical properties of the modulator, which are carried out by the deformable layer 34. This allows the structural design and materials used for the reflective layer 14 to be optimized with respect to the optical properties, and the structural design and materials used for the deformable layer 34 to be optimized with respect to desired mechanical properties.
[0054] As mentioned above, interferometric modulators, such as those depicted in Figures 7A-7E, may be manufactured by using a sacrificial layer to define the air gaps. As a last step of manufacture, the sacrificial layer may be removed by etching (herein referred to as "releasing" an interferometric modulator). Suitable materials for the sacrificial layer include, but are not limited to, molybdenum, germanium, tungsten, and amorphous silicon.
[0055] Figure 8 is a cross-sectional view illustrating an embodiment of an unre leased interferometric modulator 100 comprising a sacrificial layer 102, an upper reflective layer 14 over the sacrificial layer 102, and an etch stop layer 104 between the sacrificial layer 102 and the upper reflective layer 14. A similar structure may be used for
other MEMS devices where upper reflective layer 14 is generally an electrode layer that is preferably movable upon removal of the sacrificial layer 102. The unreleased interferometric modulator 100 corresponds to the released interferometric modulator depicted in Figure 7D (i.e., the interferometric modulator of Figure 7D is formed after release etch(es) to remove the sacrifical layer 102 and the etch stop layer 104). The etch stop layer 104 may be used to protect the sacrificial layer 102 during patterning of the reflective layer 14. For example, when the reflective layer 14 is aluminum and the sacrificial layer 102 is molybdenum, the etchant used to pattern the reflective layer 14 (e.g., a PAN etchant) may also partially etch the underlying sacrificial layer 102 unless the etch stop layer 104 is included. The skilled artisan will appreciate that this problem will also exist with other combinations of materials and etchants.
[0056] In one embodiment, the thickness of the etch stop layer 104 may be in the range of about 100 A to about 700 A. In some embodiments, the thickness of the etch stop layer 104 is in the range of about 300 A to about 700 A. Etch stop layers 104 consisting of SiO2 or titanium may be used, for example, as discussed more fully in co- pending U.S. Application No. 11/090,773, filed March 25, 2005, which is incorporated herein by reference in its entirety. However, SiO2 is not completely removed by the XeF2 used to remove the sacrificial layer 102, leaving undesired residue on the reflective layer 14. Use of titanium tends to distort the flatness of an aluminum reflective layer 14. Accordingly, there is a need for improved etch stop layer materials. As described more fully herein, it has been surprisingly found that silicon-rich silicon nitrides provide good etch stop functionality as well as being well removed by the XeF2 etchant used to remove the sacrificial layer 102. Thus, in some embodiments, the etch stop layer 104 comprises a silicon-rich silicon nitride. In some embodiments, the silicon-rich silicon nitride etch stop layer 104 may be removed during the release etch that removes the sacrificial layer.
[0057] As used herein "silicon-rich silicon nitride" refers to any silicon nitride material that has a ratio of silicon to nitrogen greater than the typical stoichiometric silicon nitride ratio of about 3:4. The silicon-rich silicon nitride etch stop layer can be formed by chemical vapor deposition (e.g., at low temperature by plasma enhanced chemical vapor deposition) or any other suitable means. In some embodiments, the silicon-rich silicon nitride has a silicon to nitrogen ratio of greater than about 1:1. Preferably, silicon nitride films are provided that have a refractive index of greater than about 2.1. More preferably, silicon nitride films are provided that have a refractive index of greater than about 2.2.
[0058] In the illustrated embodiment, the upper reflective layer 14 (or other movable electrode layer for MEMS devices other than interferometric modulators) may be aluminum. In other embodiments, the upper reflective layer 14 may be a material that comprises aluminum and thus may be an aluminum alloy such as, for example, Al-Si, Al- Cu, Al-Ti, or Al-Nd. The sacrificial layer 102 comprises molybdenum in the illustrated embodiment. Other suitable sacrificial materials include, but are not limited to, amorphous silicon ("a-Si"), germanium, and tungsten. In some embodiments, the etch stop layer 104 also acts as a diffusion barrier to prevent interdiffusion between the material in the sacrificial layer 102 and the upper reflective layer 14. For example, where the sacrificial layer 102 is amorphous silicon and the upper reflective layer 14 is aluminum, an etch stop layer 104 of silicon-rich silicon nitride will prevent interdiffusion between the aluminum in the upper reflective layer 14 and the silicon in the sacrificial layer 102. In some embodiments, the materials used for the fabrication of the sacrificial layer 102, the reflective layer 14, and the etch stop layer 104 are selected in combination with one another to bring about certain desired effects such as etch selectivity, resistance to diffusion (diffusion barrier), barrier to crystallographic influence, and crystallographic templating, as described in greater detail below.
[0059] The upper reflective layer 14 and etch stop layer 104 are spaced from a glass substrate 20 by posts 18, which in the illustrated embodiment include support plugs 42. In other embodiments, the upper reflective layer 14 may be supported by other structures, including side walls, such as for example is depicted in Figure 7C. The unreleased interferometric modulator 100 also includes a transparent electrode layer 106 over the glass substrate 20. The electrode layer 106 may comprise a transparent metal film such as indium tin oxide (ITO) or zinc tin oxide (ZTO). A lower reflective layer 108 (such as chrome or molybdenum) and a dielectric layer 1 10 (such as a Siθ2 or a composite layer comprising a layer of SiO2 and a layer of Al2O3) are formed over the electrode layer 106. The electrode layer 106, lower reflective layer 108, and dielectric layer 110 may together be referred to as an optical stack 16 that partially transmits and partially reflects light. It will be appreciated that the etch stop layer 104 may be included in other unreleased interferometric modulator configurations, e.g., any of the configurations resulting in the interferometric modulators illustrated in Figures 7A-7E.
[0060] It has been found that the presence of an etch stop layer between the upper reflective layer and the sacrificial layer (such as the etch stop layer 104 between the
sacrificial layer 102 and the reflective layer 14) may significantly improve one or more aspects of various processes for making interferometric modulators (including arrays thereof), and/or may improve one or more qualities of the resulting interferometric modulators themselves. For example, the etch stop layer 104 may comprise or serve as an etch stop as described below with reference to Figures 9 A-I OH in the context of making an array of interferometric modulators of the general type illustrated in Figure 7D.
[0061] In view of the illustrated embodiments, those skilled in the art will understand that similar etch stop layers may be used to manufacture other MEMS devices, including interferometric modulators of the general types illustrated in Figures 7A-7E, as well as other types of spatial light modulators. In general, the etch stop layer may be used between a layer used to define a cavity (e.g., sacrificial layer 102c) and a structure adjacent to the cavity (e.g., a movable electrode such as reflective layer 14) in any MEMS device. Thus, while the process described below with respect to Figures 9A- 1OH may refer to particular steps, sequences, and materials, it is understood that such details are for the purpose of illustration, and that other steps, sequences and/or materials may be used.
[0062] Figures 9A-9E are cross-sectional views illustrating the initial steps in a process for manufacturing an array of unreleased interferometric modulators (release by removal of the sacrificial material to form interferometric modulators is discussed below with reference to Figures 10A- 10H). In Figures 9A- 1OH, the formation of an array of three interferometric modulators 200 (red subpixel), 202 (green subpixel), and 204 (blue subpixel) are illustrated. Each of the interferometric modulators 200, 202, and 204 have a different distance between the lower reflective layer 108 and the upper reflective layer 14 as indicated in Figure 1OH, which shows final configurations. Color displays may be formed by using three (or more) modulator elements to form each pixel in the resulting image. The dimensions of each interferometric modulator cavity (e.g., the cavities 206, 208, and 210 in Figure 10H) determine the nature of the interference and the resulting color. One method of forming color pixels is to construct arrays of interferometric modulators, each having cavities of differing sizes, e.g., three different sizes corresponding to red, green and blue as shown in this embodiment. The interference properties of the cavities are directly affected by their dimensions. In order to create these varying cavity dimensions, multiple sacrificial layer thicknesses may be fabricated as described below so that the resulting pixels reflect light corresponding to each of the three primary colors. Other color combinations are also possible, as well as the use of black and white pixels.
[0063] Figure 9 A illustrates an optical stack 16 formed by depositing an indium tin oxide electrode layer 106 on a transparent substrate 20 and then depositing a first reflective layer 108 on the electrode layer 106. In the illustrated embodiment, the first reflective layer 108 comprises chrome. Other reflective metals such as molybdenum and titanium may also be used to form the first reflective layer 108. In Figures 9A-10H, although the electrode layer 106 and the first reflective layer 108 are indicated as a single layer 106, 108, it is understood that for an interferometric modulator embodiment, the first reflective layer 108 is formed on the electrode layer 106 as illustrated in Figure 8. In other MEMS devices, only a single electrode layer may be required. The viewing surface 120 of the transparent substrate 20 is on the opposite side of the substrate 20 from the first reflective layer 108 and the electrode layer 106. In a process not shown here, the electrode and first reflective layers 106, 108 are patterned and etched to form electrode columns, rows, or other useful shapes as required by the display design. As indicated in Figure 9A, the optical stack 16 also includes an oxide dielectric layer 1 10 over the reflective layer 108, typically formed after the electrode and first reflective layers 106, 108 have been patterned and etched.
[0064] Figure 9 A further illustrates a first subpixel sacrificial layer 102a formed by depositing molybdenum over the optical stack 16 (and thus over the oxide dielectric layer 110, first reflective layer 108, and electrode layer 106). The molybdenum is etched to form the first pixel sacrificial layer 102a, thereby exposing a portion HOa of the oxide dielectric layer 1 10 that is the region where the resulting green and blue interferometric modulators 202 and 204 are formed (Figure 10H). The thickness of the first sacrificial layer 102a (along with the thicknesses of subsequently deposited layers as described below) influences the size of the corresponding cavity 206 in the resulting red interferometric modulator 200 (Figure 10H).
[0065] Figures 9B-9C illustrate forming a second subpixel sacrificial layer 102b by deposition, masking, and patterning over the exposed portion 110a of the oxide dielectric layer 110 and the first subpixel sacrificial layer 102a. The second subpixel sacrificial layer 102b preferably comprises the same sacrificial material as the first subpixel sacrificial layer 102a (molybdenum in this embodiment). The second subpixel sacrificial layer 102b is patterned and etched as illustrated in Figure 9C to expose a portion HOb of the oxide dielectric layer 110 in the region where the resulting blue interferometric modulator 204 will be formed (Figure 10H).
[0066] A third subpixel sacrificial layer 102c is then deposited over the exposed portion 1 10b of the oxide dielectric layer 110 and the second subpixel sacrificial layer 102b as illustrated in Figure 9D. The third subpixel sacrificial layer 102c need not be patterned or etched in this embodiment, since its thickness will influence the sizes of all three cavities 206, 208, and 210 in the resulting interferometric modulators 200, 202, and 204 (Figure 10H). The three deposited subpixel sacrificial layers 102a5 102b, and 102c do not necessarily have the same thickness. In the illustrated embodiment, the thicknesses of the sacrificial layers 102a, 102b, and 102c cumulatively define the air gap 206 of the red subpixel 200 (Figure 10H). The thicknesses of the sacrificial layers 102b and 102c cumulatively define the air gap 208 of the green subpixel 202 (Figure 10H). The thickness of the sacrificial layer 102c defines the air gap 210 of the blue subpixel 204 (Figure 10H).
[0067] Figure 9E illustrates forming an etch stop layer 104 by depositing silicon-rich silicon nitride as described above over the third subpixel sacrificial layer 102c, followed by depositing a second reflective layer 14 (e.g., an aluminum-containing metal) over the etch stop layer 104. In the illustrated embodiment, the second reflective layer 14 also serves as an electrode. The second reflective layer 14 is preferably deposited immediately or very soon after the etch stop layer 104 is deposited. In one embodiment, the second reflective layer 14 is deposited over the etch stop layer 104 immediately after depositing the etch stop layer 104, preferably in the same deposition chamber and without breaking a vacuum, resulting in reduced oxidation of the surface of the second reflective layer 14. The thickness of the etch stop layer 104 may be in the range of about 100 A to about 700 A, preferably in the range of about 100 A to about 300 A. For embodiments in which the etch stop layer 104 is also a diffusion barrier, the thickness of the etch step layer is preferably in the range of from about 300 A to about 700 A. Although the foregoing description refers to certain exemplary materials for the fabrication of the various layers illustrated in Figures 9A- 1OH, it will be understood that other materials may also be used, e.g., as described above with reference to Figure 8.
[0068] Figures 1 OA-I OH are cross-sectional views illustrating various later steps following the process steps illustrated in Figures 9A-9E. In Figure 1OA, the second reflective layer 14 (comprising aluminum in this embodiment) has been patterned and etched using an appropriate etch chemistry for the removal of the metal. Such etch chemistries are known to those skilled in the art. For example, a PAN etchant (aqueous phosphoric acid/acetic acid/nitric acid) may be suitable for removing the metal. Remaining
portions 14a, 14b, and 14c of the second reflective layer 14 are protected by a mask (not shown) and thus are not removed during etching. During etching of the second reflective layer 14 to form the second reflective layer portions 14a, 14b, and 14c, the etch stop layer 104 protects the underlying third sacrificial layer 102c from being etched. Etching of the second reflective layer 14 to form the portions 14a, 14b, and 14c exposes portions 104a of the etch stop layer 104. Unexposed portions 104b of the etch stop layer 104 underlie the remaining second reflective layer portions 14a, 14b, and 14c. The exposed portions 104a of the etch stop layer 104 may then optionally be removed (Figure 10B) by further etching using a different etch chemistry (e.g., a hydrofluoric acid (HF) etchant or buffered oxide etchants (BOE) (i.e., blends of HF and ammonium fluoride)) that does not remove the third sacrificial layer 102c so that the portions 104b underlying the remaining metal reflective layer 14a, 14b, and 14c remain. Removal of the exposed portions 104a of the etch stop layer 104 ensures that no etch stop layer 104 material remains between sacrificial layers. This result permits use of etchants that do not etch the etch stop layer 104 material for patterning the sacrificial layers, such as to form post holes as described below. For example, most wet etchants that etch molybdenum do not etch silicon nitrides.
[0069] Figure 1OB illustrates the formation of a fourth sacrificial layer 102d over the patterned second reflective layer 14 a, 14b, and 14c and the third sacrificial layer 102c. Figure 1OC illustrates forming connector holes 122a and post holes 122b by patterning and etching the sacrificial layers 102a, 102b, 102c, and 102d. In Figure 10D, a planarization material 124 is optionally applied to fill in the connector holes 122a and post holes 122b. Examples of planarization materials include, but are not limited to, silicon dioxide, silicon nitride, organic materials (e.g., epoxies, acrylics, and vinyl-based chemistries), and silicon- or metal-containing organometallics. In one embodiment, various polyimides, low-k materials, and spin-on glasses may be used. Figure 1OE illustrates forming a mechanical film (flex or deformable layer) 34 by depositing a flexible material such as a metal over the planarization material 124 and the fourth sacrificial layer 102d, followed by patterning and etching the mechanical layer 34 to form columns or rows such that an array of unreleased interferometric modulators 130 is formed (Figure 10F). In an embodiment (not shown), the planarization material 124 is not used, in which case the connector holes 122a and post holes 122b may be filled with the same material that is used to form the mechanical layer 34.
[0070] Figure 1OG illustrates removing the sacrificial layers 102a, 102b, 102c, and 102d to form the cavities 206, 208, 210, thereby exposing the portion 104b of the etch stop layer 104 underlying the remaining portions 14a, 14b, and 14c of the reflective layer 14. In this embodiment, the etch stop layer 104a underlying the second reflective layers 14a, 14b, and 14c that is exposed by the removal of the sacrificial layers 102a, 102b, 102c may be used to protect the second reflective layers 14a, 14b, and 14c during the etching of the sacrificial layers 102a, 102b, 102c, and 102d. For this embodiment, etchants may be used that etch the sacrifϊcal layer material but not the etch stop layer material. For example, most wet etchants that etch molybdenum do not etch silicon nitrides.
[0071] The planarization material 42 is not removed by the etchant and thus remains to form posts 42 (Figure 10H). The etch stop layer 104b underlying the second reflective layer 14a, 14b, and 14c may then itself be removed by etching using an appropriate etch chemistry (e.g., SF6 plasma etch) as illustrated in Figure 1OH, thereby exposing the mirror surface of the second reflective layer 14a, 14b, and 14c.
[0072] Alternatively, gaseous or vaporous XeF2 is used as an etchant to remove both the molybdenum sacrificial layers 46a, 46b, 46c, 46d and the etch stop layer 104b simultaneously. For example, as described further below, it has been surprisingly discovered that silicon-rich silicon nitride may be completely removed using a XeF2 etch. It will be understood that XeF2 may serve as a source of fluorine-containing gases such as F2 and HF, and thus F2 or HF may be used in place of or in addition to XeF2 as an etchant for the preferred sacrificial materials, including molybdenum, amorphous silicon, germanium, and tungsten.
[0073] A comparison of Figures 1OH and 9E illustrates that the size of the cavity 206 (Figure 10H) corresponds to the combined thicknesses of the three sacrificial layers 102a, 102b, and 102c and the etch stop layer 104. Likewise, the size of the cavity 208 corresponds to the combined thickness of two sacrificial layers 102b and 102c and the etch stop layer 104, and the size of the cavity 210 corresponds to the combined thicknesses of the sacrificial layer 102c and the etch stop layer 104. Thus, the dimensions of the cavities 206, 208, and 210 vary according to the various combined thicknesses of the four layers 102a, 102b, 102c, and 104, resulting in an array of interferometric modulators 200, 202, and 204 capable of displaying three different colors such as red, green and blue.
[0074] The materials used for the fabrication of the sacrificial layer(s) 102, the reflective layer 14, and the etch stop layer 104 are preferably selected in combination with
one another to bring about certain desired effects. In one embodiment, the etch stop layer 104 also serves as a diffusion barrier layer that slows diffusion of metal from the reflective layer 14 into the sacrificial material 102. It has been found that such diffusion is often undesirable because it tends to blur the boundary between the reflective layer and the sacrificial layer, resulting in reduced etch selectivity during processing and reduced mirror quality in the resulting interferometric modulator. The etch stop layer/barrier layer 104 preferably has a thickness in the range of about 300 A to about 700 A.
[0075] In one embodiment, the etch stop layer 104 also serves as a buffer layer that substantially prevents a crystallographic orientation of the sacrificial material 102 from producing a corresponding crystallographic orientation in the reflective layer 14. It has been found that some materials used to form the sacrificial layer display a crystallographic orientation after deposition and/or subsequent processing steps. For example, molybdenum is a crystalline material having a crystallographic orientation (typically body centered cubic) on any particular surface that results from the crystalline lattice spacing of the molybdenum atoms. When a reflective layer 14 is deposited directly onto a molybdenum sacrificial material 102, the depositing metal may tend to follow the crystallographic orientation of the underlying molybdenum, producing a corresponding crystallographic orientation in the reflective layer 14. The lattice spacing of the resulting deposited metal layer is often different than it would be in the absence of the underlying molybdenum, and in many cases the deposited metal layer is mechanically strained as a result. Upon removal of the sacrificial layer, the as-deposited lattice spacing of the metal atoms may relax to the natural lattice spacing for the metal, in some cases changing the dimensions of the reflective layer and producing undesirable warping.
[0076] For embodiments in which the etch stop layer 104 also serves as a buffer layer, the etch stop layer/buffer layer 104 is preferably amorphous or does not have the same lattice spacing as the underlying sacrificial layer 102. For example, silicon-rich silicon nitride is typically amorphous. The metal atoms deposit on the etch stop layer/buffer layer 104 rather than on the underlying sacrificial layer 102, and the buffer layer substantially prevents a crystallographic orientation of the sacrificial layer 104 from producing a corresponding crystallographic orientation in the reflective layer 14.
[0077] In one embodiment, the etch stop layer 104b also serves as a template layer having a crystalline orientation that is substantially similar to a crystallographic orientation of the reflective layer 14. As discussed above, a depositing metal may tend to
follow the crystallographic orientation of the underlying layer, producing a corresponding crystallographic orientation in the metal layer. This tendency may be used to advantage by selecting, for use as an etch stop layer 104, a material that has a crystallographic orientation that would be desirable to impart to the reflective layer 14. An etch stop layer 104 formed of such a material thus serves as a crystallographic template that produces a substantially similar crystalline orientation in the subsequently deposited reflective layer 14.
[0078] The processing steps used to fabricate the interferometric modulators and arrays thereof described herein are preferably selected in combination with the materials used for the fabrication of the sacrificial layer 102, the reflective layer 14, and the etch stop layer 104 to bring about certain desired effects. For example, in one embodiment described above with reference to Figure 1 OA, during etching of the second electrode or reflective layer 14 to form the portions 14a, 14b, and 14c, the etch stop layer 104 protects the underlying third sacrificial layer 102c from being etched. In another embodiment described above with reference to Figure 1OG. the etch stop layer 104b (underlying the second electrode or mirror layers 14a, 14b, and 14c) that is exposed by the removal of the sacrificial layers 102a, 102b, 102c protects the second mirror layers 14a, 14b, and 14c during the etching of the sacrificial layers 102a, 102b, 102c, 102d. Thus, the etch stop layer 104 may protect a sacrificial layer and/or a reflective layer from being etched during the removal of some other layer. During such etching, the material being etched is preferably removed at a rate that is at least about 10 times faster than the rate at which the etch stop layer is removed, preferably at least about 20 times faster. Thus, for example, with reference to Figure 1OA, during etching of the second reflective layer 14 to form the portions 14a, 14b, and 14c, the aluminum in the second reflective layer 14 is preferably removed by the etchant at a rate that is at least about 10 times faster than the rate at which the material in the etch stop layer 104 is removed by the etchant, and more preferably at least about 20 times faster. Likewise, with reference to Figure 1OG, if the etch stop layer 104 is not to be removed simultaneously with the sacrificial layer(s), during etching of the sacrificial layers 102a, 102b, 102c, and 102d, the material in the sacrificial layers is preferably removed at a rate that is at least about 10 times faster than the rate at which the material in the etch stop layer 104 is removed, and more preferably at least about 20 times faster.
[0079] With reference to Figures 1 OG-I OH, the portions 104b of the etch stop layer 104 underlying the second electrode or reflective layer portions 14a, 14b, and 14c
may be selectively removed by etching to expose the mirror surfaces of the second reflective layer portions 14a, 14b, and 14c in a manner that minimizes damage to the mirror surfaces. The etchant preferably removes the portions 104b of the etch stop layer 104 at a rate that is at least about 10 times faster than a rate at which the etchant removes the second mirror reflective layer portions 14a, 14b, and 14c, more preferably at least about 20 times faster.
[0080] The above embodiments are not intended to limit the present invention, and the methods described herein may be applied to any structure in which two materials having similar etching profiles are used in a proximate area and subjected to etching where selective etching is desired. Preferably, the methods described herein may be applied to increase etch selectivity between combinations of an Al-containing material and a Mo- containing material. No structural limitation or restriction is imposed or intended. Further, no limitation or restriction is imposed or intended on the particular formation sequence.
[0081] The methods described herein for the fabrication of interferometric modulators may use conventional semiconductor manufacturing techniques such as photolithography, deposition (e.g., "dry" methods such as chemical vapor deposition (CVD) and wet methods such as spin coating), masking, etching (e.g., dry methods such as plasma etch and wet methods), etc.
EXAMPLES Example 1
[0082] A thin film of standard silicon nitride (silicon to nitrogen ratio of 3:4) formed on a substrate was tested for sensitivity to various etchants including PAD, PAN and XeF2 etchants. A test pattern mask was applied to the standard silicon nitride films and the films were exposed to the etchants. After removing the pattern mask, any resulting step height was measured to determine sensitivity to the etchants. Exposure to the PAD etchant was at room temperature for a 10 minute soak. The standard silicon nitride film was only very slightly etched by the PAD etchant. Exposure to XeF2 consisted of using two cycles of 120 s of gas fill time followed by 300 s of etching time. No etching of the standard silicon nitride was observed. Exposure to the PAN etchant was at room temperature for a 10 minute soak. No etching of the standard silicon nitride was observed. Thus, standard silicon nitride is not sensitive to PAD, PAN, or XeF2 etchants.
Example 2
[0083] Test wafers were constructed using five different deposition conditions to form various silicon nitride films on glass or silicon wafers. The silicon nitride films were formed by Micralyne, Inc. of Edmonton Alberta using plasma enhanced chemical vapor deposition (PECVD) by reaction between SiH4 and NH3. All silicon nitride films were formed at a pressure of 900 mTorr and a temperature of 350 0C. RF power for generating the plasma was 20 W. The gas flow rates, deposition rates (DR), and measured refractive indices (RI) of the resulting films are indicated in Table 1.
[0084] The sensitivities of these test films to etching by XeF2 and PAN etchants were determined by applying a test pattern mask and then exposing the films to the respective etchants. The pattern mask was then removed and any resulting step heights measured. The XeF2 etch test consisted of exposing the five films formed on glass wafers to two cycles of 120 s XeF2 gas fill time followed by 300 s of etch time. The PAN etch test consisted of soaking the five films formed on silicon wafers in PAN etchant for 10 minutes. The PAN etchant resulted in no observable etching of any of the silicon nitride films. In contrast, the silicon-rich silicon nitride films (e.g., those formed by reaction conditions 2-5) were sensitive to XeF2 etching. Table 2 lists the observed step heights formed from XeF2 etching of the test pattern.
Table 2. Step hei hts caused b XeF2 etchin .
[0085] Figure 11 depicts a graph showing the observed step height as a function of refractive index. Also included in the graph is the standard silicon nitride tested in Example 1, with a refractive index of about 1.9. This data indicates that as the refractive index increases, the sensitivity to XeFa etching generally increases. The refractive index of standard silicon nitride (i.e., a 3:4 ratio of silicon to nitrogen) is approximately 1.9 to 2.1. The refractive index of pure silicon is 3.7. Accordingly, increasing refractive indices above 2.1 indicate increasing amounts of silicon in the silicon nitride films (e.g., silicon-rich silicon nitride). These increasing refractive indices also correlate with the increase in SiH4/NH3 reactant ratios (Table 1). Thus, unlike standard silicon nitride (i.e., a 3:4 ratio), silicon-rich silicon nitride films are sensitive to XeFz etching and can therefore be cleanly removed during XeF2 release etching in interferometric modulators.
Example 3
[0086] Test wafers were constructed using four different deposition conditions to form various silicon nitride films on glass or silicon substrates. The silicon nitride films were formed using plasma enhanced chemical vapor deposition by reaction between SiHU and NH3. All silicon nitride films were formed at a pressure of 650 mTorr. RF power for generating the plasma was 25 W. The gas flow rates, temperature, deposition rates (DR), and measured refractive indices (Rl) of the resulting films are indicated in Table 3. Condition 1 corresponds to deposition conditions resulting in standard silicon nitride (i.e., a silicon to nitrogen ratio of 3:4). Condition 4 corresponds to the standard conditions except for a lower reaction temperature. Increasing the ratio of the SiH4 reactant to NH3 resulted in an increase in refractive index, indicating an increase in the silicon content of the resulting film.
[0087] The sensitivities of these test films to etching by XeF2 and PAN etchants were determined by applying a test pattern mask and then exposing the films to the respective etchants. The pattern mask was then removed and any resulting step heights
measured. The XeF2 etch, test consisted of exposing the four films to four cycles of 120 s XeF2 gas fill time followed by 300 s of etch time. The PAN etch test consisted of soaking the four films in PAN etchant for 10 minutes. The PAN etchant resulted in no observable etching of the silicon nitride films. On glass wafers, standard silicon nitride (e.g., wafer no. 1) also showed no observable etching as a result of exposure to XeF2. In contrast, silicon- rich silicon nitride films on glass wafers (e.g., wafer nos. 2 and 3) were sensitive to XeF2, resulting in measurable step heights where the film was etched. The wafer no. 4 silicon nitride films showed some sensitivity to XeF2 etching, however, the resulting step heights were not consistent.
[0088] All of the silicon nitride films were sensitive to XeF2 etching on a silicon substrate, however, standard silicon nitride (e.g., wafer no. 1) was not completely removed. In contrast, the silicon-rich silicon nitride films on silicon substrates were completely removed upon XeF2 etching.
[0089] It will be appreciated by those skilled in the art that various omissions, additions and modifications may be made to the processes described above without departing from the scope of the invention, and all such modifications and changes are intended to fall within the scope of the invention, as defined by the appended claims.
Claims
1. An unreleased MEMS device, comprising: a silicon nitride layer positioned between a sacrificial layer and an electrode layer, wherein the electrode layer is adapted to be movable upon removal of the sacrificial layer and the ratio of silicon to nitrogen in the silicon nitride layer is greater than 3:4.
2. The unreleased MEMS device of claim 1, wherein the electrode layer is positioned over the sacrificial layer and a substrate underlies the sacrificial layer.
3. The unreleased MEMS device of claim 1 or 2, wherein the unreleased MEMS device is an unreleased interferometric modulator and the electrode layer comprises a metal mirror.
4. The unreleased MEMS device of any one of claims 1-3, wherein the ratio of silicon to nitrogen in the silicon nitride layer is greater than about 1:1.
5. The unreleased MEMS device of any one of claims 1-4, wherein the sacrificial layer is sensitive to removal by a XeF2 etchant.
6. The unreleased MEMS device of any one of claims 1-5, wherein the sacrificial layer comprises a material selected from the group consisting of amorphous silicon, germanium, molybdenum, and tungsten.
7. The unreleased MEMS device of any one of claims 1-6, wherein the silicon nitride layer is sensitive to removal by an etchant that is also capable of removing the sacrificial layer.
8. The unreleased MEMS device of any one of claims 1-7, wherein the electrode layer comprises aluminum.
9. The unreleased MEMS device of any one of claims 1-8, wherein the silicon nitride layer is adapted to substantially prevent interdiffusion between the electrode layer and the sacrificial layer.
•10. The unreleased MEMS device of any one of claims 1-9, wherein the silicon nitride layer is adapted to substantially prevent a crystallographic orientation of the sacrificial layer from producing a corresponding crystallographic orientation in the electrode layer.
11. The unreleased MEMS device of any one of claims 1-10, wherein the silicon nitride layer has a refractive index greater than about 2.1.
12. The unreleased MEMS device of any one of claims 1-11, wherein the silicon nitride layer has a refractive index greater than about 2.2.
13. The unreleased MEMS device of any one of claims 1-12, wherein the sacrificial layer is selected from the group of molybdenum and amorphous silicon and the electrode layer comprises aluminum.
14. An unreleased interferometric modulator, comprising: an etch stop layer positioned between a sacrificial layer and a metal mirror layer, wherein the metal mirror layer is adapted to be movable upon removal of the sacrificial layer and the etch stop layer is adapted to be substantially completely removed upon exposure to XeF2 for less than about 10 minutes.
15. The unreleased interferometric modulator of claim 14, wherein the metal mirror layer is positioned over the sacrificial layer.
16. The unreleased interferometric modulator of claim 14 or 15, wherein the etch stop layer comprises a silicon nitride.
17. The unreleased interferometric modulator of any one of claims 14-16, wherein the sacrificial layer is also adapted to be substantially completely removed upon exposure to XeF2.
18. The unreleased interferometric modulator of any one of claims 14-17, wherein the sacrificial layer is selected from the group consisting of molybdenum and amorphous silicon and the electrode layer comprises aluminum.
19. An unreleased MEMS device, comprising: a silicon nitride layer positioned between a sacrificial layer and an electrode layer, wherein the electrode layer is adapted to be movable upon removal of the sacrificial layer, the silicon nitride layer is adapted to be substantially completely removed upon exposure to a first etchant that is adapted to substantially completely remove the sacrificial layer, and the silicon nitride layer is adapted to be substantially resistant to a second etchant that is adapted to etch the electrode layer.
20. The unreleased MEMS device of claim 19, wherein the electrode layer is positioned over the sacrificial layer.
21. The unreleased MEMS device of claim 19 or 20, wherein the unreleased MEMS device is an unreleased interferometric modulator and the electrode layer comprises a metal mirror.
22. The unreleased MEMS device of any one of claims 19-21, wherein the sacrificial layer is selected from the group consisting of molybdenum and amorphous silicon and the electrode layer comprises aluminum.
23. The unreleased MEMS device of any one of claims 19-22, wherein the first etchant is XeF2. '
24. The unreleased MEMS device of any one of claims 19-23, wherein the second etchant is PAN.
25. An unreleased interferometric modulator, comprising: means for reflecting light; means for supporting the reflecting means during interferometric modulator manufacture; and means for protecting the supporting means during etching of the reflecting means.
26. The unreleased interferometric modulator of claim 25, wherein the reflecting means is a metal mirror.
27. The unreleased interferometric modulator of claim 25 or 26, wherein the supporting means is a sacrificial layer.
28. The unreleased interferometric modulator of any one of claims 25-27, wherein the protecting means is a silicon nitride layer and wherein the ratio of silicon to nitrogen in the silicon nitride layer is greater than about 3:4.
29. The unreleased interferometric modulator of any one of claims 25-28, wherein the ratio of silicon to nitrogen in the silicon nitride layer is greater than about 1 :1.
30. A method of manufacturing a MEMS device, comprising: forming a sacrificial layer; forming an electrode layer, wherein the electrode layer is adapted to be movable upon removal of the sacrificial layer; forming a silicon nitride layer between the sacrificial layer and the electrode layer, wherein the ratio of silicon to nitrogen in the silicon nitride layer is greater than about 3:4; patterning the electrode layer; and removing the sacrificial layer.
31. The method of claim 30, wherein the MEMS device is an interferometric modulator and the electrode layer comprises a metal mirror.
32. The method of claim 30 or 31 , wherein the ratio of silicon to nitrogen in the silicon nitride layer is greater than about 1 :1.
33. The method of any one of claims 30-32, wherein forming the sacrificial layer comprises depositing a material selected form the group consisting of molybdenum, amorphous silicon, germanium, and tungsten.
34. The method of any one of claims 30-33, wherein forming the silicon nitride layer comprises reacting silane with ammonia on a surface of the sacrificial layer.
35. The method of any one of claims 30-33, wherein forming the silicon nitride layer comprises depositing silicon nitride on a surface of the sacrificial layer using physical vapor deposition.
36. The method of any one of claims 30-35, wherein forming the electrode layer comprises depositing aluminum onto the silicon nitride layer.
37. The method of any one of claims 30-36, wherein patterning the electrode layer comprises etching the electrode layer using an etchant that does not remove the silicon nitride layer.
38. The method of any one of claims 30-37, wherein removing the sacrificial layer comprises etching the sacrificial layer with an etchant that also removes the silicon nitride layer.
39. The method of any one of claims 30-38, further comprising patterning the silicon nitride layer after patterning of the electrode layer and prior to removing the sacrificial layer.
40. A MEMS device manufactured by the process of any one of claims 30-39.
41. An interferometric modulator manufactured by the process of any one of claims 30-39.
42. A method of manufacturing a MEMS device, comprising: forming a sacrificial layer; forming an electrode layer, wherein the electrode layer is adapted to be movable upon removal of the sacrificial layer; forming an etch stop layer between the sacrificial layer and the electrode layer; patterning the electrode layer; and removing the sacrificial layer and etch stop layer with a same etchant.
43. The method of claim 42, wherein the etch stop layer comprises a silicon nitride.
44. The method of claim 43, wherein the etch stop layer has a refractive index greater than about 2.1.
45. The method of any one of claims 42-44, wherein the MEMS device is an interferometric modulator and the electrode layer comprises a metal mirror.
46. The method of any one of claims 42-45, where the etchant comprises xenon fluoride.
47. The method of any one of claims 42-46, wherein: forming the sacrificial layer comprises depositing a material selected from the group consisting of molybdenum, amorphous silicon, germanium, and tungsten; forming the etch stop layer comprises forming silicon nitride on the sacrificial layer; and forming the electrode layer comprises depositing aluminum onto the silicon nitride.
48. A MEMS device manufactured by the process of any one of claims 42-47.