WO2009026298A1 - Mask trimming - Google Patents
Mask trimming Download PDFInfo
- Publication number
- WO2009026298A1 WO2009026298A1 PCT/US2008/073602 US2008073602W WO2009026298A1 WO 2009026298 A1 WO2009026298 A1 WO 2009026298A1 US 2008073602 W US2008073602 W US 2008073602W WO 2009026298 A1 WO2009026298 A1 WO 2009026298A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- mask
- deposition
- recited
- etching
- deposition layer
- Prior art date
Abstract
Description
Claims